Aluminum alloy reference

Registered composition limits, usual tempers, forms, standards, and applications for the alloys we work with most. A reference for writing a specification, not a substitute for the mill test certificate.

Both directions

How to use this page

Limits are maximum percentages by weight unless a range is shown; others 0.05 each, 0.15 total, except the 1xxx grades, where 1050 and 1070 carry others 0.03 each with no total and a vanadium limit of 0.05; balance aluminum.

This page lists the alloys and grades Inquivix Technologies works with most often, grouped by family, with the registered composition limits, the tempers and forms in which Korean mills and overseas producers normally supply them, the standards that govern them, and the applications they serve. It is a reference for writing a specification, not a substitute for the mill test certificate, which is the only document that states the chemistry of the metal you receive.

Composition limits are the Aluminum Association registered limits as published in the international alloy designation system. KS, ASTM, EN, and JIS designations for these alloys are harmonised to the same limits in nearly all cases, and the mill certificate will state which standard was applied. For a product inquiry, state the alloy, the temper, the form, the standard, and the dimensions; the rolled products page explains the full specification sequence.

Primary metal grades

GradeAl minSi maxFe maxNotes
P102099.700.100.20Standard LME-deliverable primary ingot (P1020A). The designation reads P, then the Si maximum, then the Fe maximum
A799.700.150.16GOST 11069 primary grade from CIS smelters; accepted as P1020-equivalent by most mills
P061099.85 by trade convention0.060.10Higher purity for electrical and foil applications (P0610A)

Forms: standard ingot (approximately 20 to 25 kg), T-bar, sow. Direction: into Korea. Standards: LME contract specification; producer specification; KS D 2304 for aluminum ingot.

1xxx: commercially pure

AlloySiFeCuMnMgCrZnTiAl min
10500.250.400.050.050.050.050.0399.50
10700.200.250.040.030.030.040.0399.70
11000.95 Si+Fe0.05 to 0.200.050.1099.00

Usual tempers: O, H12, H14, H16, H18, H22, H24, H26. Forms: Coil, sheet, foil, foil stock. Direction: From Korea. Standards: KS D 6701, ASTM B209/B209M (1100; 1050 and 1070 are specified to EN or JIS), ASTM B479 (foil), EN 485 and EN 573, EN 546 (foil), JIS H4000, JIS H4160 (foil).

Applications. Electrical conductor and busbar, chemical and food process equipment, heat exchanger fin stock, lithographic sheet, household and packaging foil, battery current collector foil (1060 and 1070 class, to a separate cleanliness and tensile specification).

3xxx: manganese alloys

AlloySiFeCuMnMgCrZnTi
30030.60.70.05 to 0.201.0 to 1.50.10
30040.300.70.251.0 to 1.50.8 to 1.30.25
31040.60.80.05 to 0.250.8 to 1.40.8 to 1.30.250.10
31050.60.70.300.30 to 0.80.20 to 0.80.200.400.10

3104 also limits gallium and vanadium to 0.05 each.

Usual tempers: O, H12, H14, H16, H18, H22, H24, H26; H19 for can body stock. Forms: Coil, sheet. Direction: From Korea. Standards: KS D 6701, ASTM B209/B209M (3003, 3004, 3105; 3104 is specified to EN or JIS), EN 485 and EN 573, JIS H4000.

Applications. 3003 for general sheet metal, roofing, heat exchanger tube and fin, cooking equipment, and chemical equipment. 3004 and 3104 for beverage can body stock. 3105 for roofing, siding, and general sheet work needing more strength than 3003.

5xxx: magnesium alloys

AlloySiFeCuMnMgCrZnTi
50520.250.400.100.102.2 to 2.80.15 to 0.350.10
50830.400.400.100.40 to 1.04.0 to 4.90.05 to 0.250.250.15
51820.200.350.150.20 to 0.504.0 to 5.00.100.250.10

Usual tempers: O, H32, H34, H36, H38 (5052); O, H111, H112, H116, H321 (5083 plate); O, H19, H48 (5182 can end stock). Forms: Coil, sheet, plate. Direction: From Korea. Standards: KS D 6701, ASTM B209/B209M (5052, 5083; 5182 is specified to EN or JIS), ASTM B928/B928M for 5083 H116 and H321 marine plate, EN 485 and EN 573, JIS H4000; classification society approval (KR, ABS, DNV, LR) for marine plate where the application requires it.

Applications. 5052 for formed and welded sheet parts, fuel tanks, truck and trailer bodies, marine fittings, and electronic enclosures. 5083 for ship hulls and superstructures, pressure vessels, cryogenic tanks, and rail and truck structures. 5182 for beverage can ends and automotive inner body panels.

6xxx: magnesium-silicon alloys

AlloySiFeCuMnMgCrZnTi
60610.40 to 0.80.70.15 to 0.400.150.8 to 1.20.04 to 0.350.250.15
60630.20 to 0.60.350.100.100.45 to 0.90.100.100.10

Usual tempers: T4, T6, T651 (plate); T5, T6 (extrusions from billet). Forms: Plate; extrusion billet. Direction: Both directions (billet into Korea for extruders; plate and billet from Korea). Standards: KS D 6701 (plate), ASTM B209/B209M (plate), ASTM B221 (extrusions), EN 485 and EN 573, EN 755 (extrusions), JIS H4000, JIS H4100 (extrusions).

Applications. 6061 for structural plate, tooling and jig plate, machined components, transport structures, and marine. 6063 for architectural extrusions, window and door frames, heat sinks, and general sections where surface finish matters more than strength.

8xxx: foil alloys

AlloySiFeCuMnMgCrZnTi
80110.50 to 0.90.6 to 1.00.100.200.050.050.100.08
80210.151.2 to 1.70.05
80790.05 to 0.300.7 to 1.30.050.10

Usual tempers: O for converter foil; H18 and H19 for hard foil; H14 and H24 for container stock. Forms: Foil and foil stock. Direction: From Korea. Standards: ASTM B479, EN 546 and EN 573, JIS H4160, KS D 6705.

Applications. 8011 for household foil, closures, and general flexible packaging. 8079 for thin flexible packaging laminates and pharmaceutical blister. 8021 for blister lidding, semi-rigid containers, and applications needing higher strength at gauge.

Scrap grades

Scrap is traded by ISRI grade (now published as the ReMA Scrap Specifications Circular; the trade still says ISRI) rather than by alloy designation, and the grade names describe the sorting and source rather than a chemistry. The grades Korean mills and foundries most often seek from overseas:

ISRI (ReMA) gradeDescriptionTypical use in Korea
Clean new sheet and clipOffcuts and trim from stamping and fabrication, segregated by alloy, free of coatings and contaminationDirect return to the same alloy family in rolling mills
Taint/TaborClean mixed old alloy sheetSecondary alloy production, 3xxx and 5xxx remelt with sorting
TenseClean mixed old alloy castFoundry secondary alloys
Taldon / TaldackBaled or densified used beverage cansCan stock remelt, where the mill has UBC capability
Talon / TasteBare pure (EC-grade) aluminum wire and cable scrap, new (Talon) or old (Taste)Conductor-grade remelt
TalkAluminum-copper radiators, cleanSecondary alloy and foundry feed after separation
Segregated extrusion scrap (6063, 6061)Clean extrusion offcuts and dismantled sections, painted or unpainted statedExtrusion billet remelt

Scrap supplied into Korea is accompanied by a sorting and processing description, radioactivity screening, moisture declaration, and the import classification confirmed per shipment. Recovery rate, not nominal grade, sets the price, and it is established on the trial lot. See the primary metal page for the qualification sequence.

Temper designations in brief

CodeMeaning
FAs fabricated, no control of mechanical properties
OAnnealed, softest condition
H1xStrain hardened only (H12 quarter hard, H14 half hard, H16 three-quarter hard, H18 full hard, H19 extra hard)
H2xStrain hardened and partially annealed, better ductility at similar strength to H1x
H3xStrain hardened and stabilised; standard for 5xxx to prevent age softening
H11xH111: slightly strain hardened after annealing. H112: properties acquired from hot working, no special control. Both common for 5083 plate
H116, H321Marine tempers for 5083 with controlled corrosion resistance
T4Solution heat treated and naturally aged
T5Cooled from hot working and artificially aged (extrusions)
T6Solution heat treated and artificially aged
T651T6 and stress relieved by stretching (plate)

Standards referenced on this site

StandardCovers
KS D 6701Aluminum and aluminum alloy sheets, plates, and strips (Korea)
KS D 2304Aluminum ingot (Korea)
KS D 6705Aluminum and aluminum alloy foil (Korea)
ASTM B209/B209MAluminum and aluminum alloy sheet and plate
ASTM B479Annealed aluminum and aluminum alloy foil for flexible barrier applications
ASTM B221Aluminum alloy extruded bars, rods, wire, profiles, and tubes
EN 573Chemical composition and form of wrought products
EN 485Sheet, strip, and plate: mechanical properties and tolerances
EN 546Foil
EN 755Extruded rod, bar, tube, and profiles
JIS H4000Aluminum and aluminum alloy sheets, strips, and plates
JIS H4100Aluminum and aluminum alloy extruded shapes
JIS H4160Aluminum and aluminum alloy foils

Have a specification or a sourcing question? Tell us the product, alloy, quantity, and direction.